"Drop-in equivalent" is a claim, not a property. Verify it in three passes — TDS line by line, COA batch data, and real-part trials — before it reaches your mold.
"Drop-in equivalent" is a claim, not a property — and it is verified in three passes, not accepted from a comparison table. Pass one checks the TDS line by line: standard, condition, and value, in that order. Pass two checks whether the COA proves the batch you receive matches the datasheet you approved. Pass three checks the only thing that finally matters: your part, in your mold, in your assembly. A grade that clears all three passes is an equivalent. A grade that clears only the first is a hypothesis with a price attached.
When a TDS line is missing its standard, the number is not comparable
Read every line of the candidate's TDS against the incumbent grade's TDS, and for each property ask three questions. Which standard? Tensile strength to ISO 527 and to a national standard are measured on different specimens at different speeds; the numbers are close, but they are not interchangeable, and a supplier who will not name the standard is asking you to compare blind. Which condition? Nylon datasheets quote dry-as-molded values unless stated otherwise, yet your part works conditioned — a candidate that looks stronger dry can land softer after moisture uptake, which is why the dry-versus-conditioned question decides so many nylon switches (we walk through it in PA66 vs PA6: how to choose). Which specimen and thickness? A UL94 rating without a thickness, an impact value without a temperature, a dielectric strength without a specimen thickness — each is half a specification. Complete the halves before you compare the numbers.
Shrinkage deserves its own line in this pass. Two compounds with identical strength data and different shrinkage are not drop-in equivalents for an existing mold; they are a tooling modification. Compare mold shrinkage early, in both flow and cross-flow directions where the data exists.
When the COA only repeats the datasheet, it proves nothing about your batch
A certificate of analysis earns its name when it reports measured results for the lot being shipped — lot number, production date, and test values that were actually measured on that lot. For a compound, the batch checks that carry information are the ones that can drift: density or specific gravity, melt flow, filler content by ash or burn-off, and moisture content on delivery. If the COA simply reprints the TDS typical values with a stamp, it certifies that the printer works. Ask, before the first order, which items are measured per lot and which are periodic — and ask for a sample COA from a recent production lot of the same grade family, so you can see the format and the spread of real values. A supplier who compounds to specification through partner lines, as we do, should still be able to put a lot-specific COA in your hands for every shipment; "documents available on request" should mean the document exists, not that it will be created when asked.
This applies to every compound family, not only the ones with complete public data. When you verify a PBT grade for connector housings or a PPSU grade for hot-water and food-contact parts, the method is identical even where the published data is thinner: demand the standard behind each value, the lot COA format, and a trial — and treat any value the supplier cannot source as unverified, whatever the brochure says.
When the trial part passes the bench but fails assembly, it is not equivalent
Real-part verification starts with a mold trial on your own tool, with the candidate processed inside its published window — drying, melt and mold temperatures from its own TDS, not copied from the incumbent. Then check, in order: critical dimensions after conditioning, not only off the tool, because nylon parts move as they absorb moisture; assembly — snap-fits, press-fits, screw bosses, ultrasonic or heat-stake joints, and gasket compression on the real mating parts; function under load — the bench test your part was designed against, run on molded parts rather than test bars; and aging spot checks proportionate to the service — a heat-aging or humidity-aging sample set held back from the trial lot, compared against incumbent parts aged the same way. Keep incumbent and candidate parts from the same trial session, labeled by lot. If a failure appears six months later, those retained parts are your evidence.
Five kilograms of trial material is usually enough for this pass: a short mold trial, a set of assembly parts, and retained samples. That is exactly what our 5 kg sample lots are sized for.
Red flags: stop and ask harder questions when you see these
- The same property quoted to different standards in the brochure and the TDS — or no standard named at all.
- Values with no condition attached: no temperature, no dry/conditioned state, no specimen thickness for electrical or flammability data.
- Ranges where the incumbent gives a typical value — a range wide enough to hide a different compound.
- A TDS that is the base-resin producer's sheet with a trader's logo on it; the compound you buy is not the resin on that sheet.
- Flame ratings quoted at a thickness your part does not have.
- A COA offered "after shipment", or one whose values are identical, lot after lot, to the second decimal.
- Processing guidance missing from the TDS — no drying, melt or mold temperatures means the trial will be run on folklore.
Any single flag can have an innocent explanation. Two or more together mean the equivalence claim is marketing, and the verification burden has just moved to you.
What a complete TDS looks like: one real example
A verifiable TDS names the standard and condition beside every value, and closes with a processing window. This is the published data structure of our PEI-NC polyetherimide grade, shown here as the pattern to demand from any supplier:
| Property | Standard | Condition | Value |
| Density | ISO 1183 | — | 1.28 g/cm³ |
| Tensile strength | ISO 527 | 23 °C | 103 MPa |
| Flexural modulus | ISO 178 | 23 °C | 6,528 MPa |
| Melt flow index | ISO 1133 | 350 °C, 5 kg | 14.5 g/10 min |
| Glass transition (Tg) | ISO 11357 | — | 220 °C |
| Flammability | UL 94 | — | V-0 |
| Dielectric strength | IEC 60243-1 | 2 mm | 30 kV/mm |
Reference values, dry, 23 °C unless otherwise stated; third-party test reports available on request.
The same sheet states its processing window — drying 150–170 °C for 4–5 hours, melt 340–360 °C, mold 150–180 °C — because a grade you cannot process from its own datasheet is not yet a grade you can verify. Whatever compound you are qualifying, ask for the sheet in this shape: every value sourced, every condition stated, nothing resting on a brochure.
Send us the grade you want to replace
Tell us the incumbent grade name or send its TDS, and we will reply with the full TDS of the closest compound we supply — in the format above — plus a 5 kg sample lot for your own three passes. Stock samples are dispatched in 1–3 working days; custom trial compounds take 10–20 working days after the specification is confirmed. Samples are charged, with freight collect. Judge the equivalence on your parts, not on our comparison table.
FAQ
Q: The supplier says the full TDS is confidential. Is that normal?
A: A public summary sheet is normal; refusing to share the full TDS under a normal commercial inquiry is not. You cannot verify what you cannot read — treat an unreadable TDS as an unverified grade.
Q: Can a good COA replace a mold trial?
A: No. A lot COA proves the batch matches the datasheet. Only a trial in your mold proves the compound matches your part — shrinkage, weld lines and assembly behavior live in the tool, not in the certificate.
Q: How much material do we need for verification?
A: For most small and medium parts, 5 kg covers a mold trial, assembly checks and retained aging samples. Larger tools or multi-cavity trials may need more — tell us the shot weight and cavity count and we will size the sample lot with you.